Abstract:
Purpose: The purpose of this in vitro study was to measure the volume loss from wear of CoCr alloy against non-precious alloy (NP), lithium disilicate (EM), advanced lithium disilicate (TR), resin-based ceramic (CM) and zirconia (ZR) after 250,000 simulated cycles. Materials and Methods: Eight flat square specimens (5 x5 x2 mm3) of each material were prepared. EM TR and ZR specimens were heat treated following the manufacturers instructions. CoCr metal alloy styli were fabricated by lost wax technique. The simulated two-body wear was performed in the oral wear simulator. The volume loss of the specimen was measured using a contact profilometer. The volume loss of the antagonist CoCr stylus was calculated by loss of height and radius of wear area. The data were analyzed statistically using MANOVA (pNP>ZR). Volume loss of styli in CM group shows less than EM and NP but the others were no significant differences.